COPYRIGHT 2000 THE ESAB GROUP, INC. LESSON
III 3/16"
200 76.4
4.85
250 74.6
5.36
300 70.3
5.61
7/32" 250
75.0
6.5 300
74.0
7.2 350
73.0
7.4 1/4"
300
78.0 7.72
350 77.0
8.67
400 74.0
9.04
*Note: Efficiencies do not include
stub loss 3.7.11
ATOM
ARC 7018AC
(AWS E7018)
- This iron powder low hydrogen electrode was
specifically designed for optimum performance
on AC power sources. This electrode features easier
arc starting, improved restrike, and smoother metal transfer than a standard E7018
electrode on AC. Typically, this
electrode is used as a tacking electrode.