97 Coreshield
10 Welding Data WIRE FEED
DEPOSITION ELECTRICAL
AMPERES VOLTS
SPEED RATE
% EFFICIENCY STICKOUT
IPM (cm/min) lbs/hr
(kg/hr) in (mm) .045"
(1.2mm) 80 13
60 (152)
1.1 (0.50)
76 1/2
(12.7) 150
17 118
(300) 2.6
(1.18) 88
1/2 (12.7)
225 18
226 (574)
5.1 (2.31)
90 1/2
(12.7) 1/16"
(1.6mm) 175 14
61 (155)
2.1 (0.95)
73 1/2
(12.7) 220
18 78
(198) 3.3
(1.50) 83
1/2 (12.7)
275 19
108 (274)
4.8 (2.18)
93 1/2
(12.7) 5/64"
(2.0mm) 250 20
58 (147)
4.0 (1.81)
94 3/4
(19.1) 300
21 85
(216) 5.1
(2.31) 85
3/4 (19.1)
400 27
143 (363)
9.2 (4.17)
90 3/4
(19.1) NOTE:
DCEN (ELECTRODE NEGATIVE) ONLY. PARAMETERS MAY VARY DEPENDING
ON MATERIAL THICKNESS. Continued
on next page... Coreshield
8Ni1 Welding Data WIRE FEED
DEPOSITION ELECTRICAL
AMPERES VOLTS
SPEED RATE
% EFFICIENCY STICKOUT
IPM (cm/min) lbs/hr
(kg/hr) in (mm) 1/16"
(1.6mm) 135 20
100 (254)
2.9 (1.3)
72 5/8
(15.9) 200
21 130
(330) 3.8
(1.7) 74
5/8 (15.9)
230 22
160 (406)
4.7 (2.1)
74 5/8
(15.9) 5/64"
(2.0mm) 170 20
65 (165)
2.8 (1.3)
71 3/4
(19.1) 195
22 80
(203) 3.4
(1.5) 72
3/4 (19.1)
230 24
100 (254)
4.7 (2.1)
73 3/4
(19.1) NOTE:
DCEN (ELECTRODE NEGATIVE) ONLY. PARAMETERS MAY VARY DEPENDING
ON MATERIAL THICKNESS.