25 Stainless
Steel Metal Core Wire Typical Mechanical
Typical Undiluted Type
Properties Weld
Metal Analysis Specifications
98 Ar/2 O2
100% Ar Arcaloy
409 Ti AWS A5.9-93
Carbon 0.02
Class EC409 Manganese
0.48 Silicon
0.55 Phosphorus
0.01 Sulfur
0.008 Chromium
11.6 Titanium
0.9 Arcaloy 409Ti
is a 12% Cr alloy stabilized with Ti for arc stability and to form carbides to
improve corrosion resistance, increase strength
at high temperatures, and promote the ferritic microstructure. Cr range
is 10.50 to 13.50%. Arcaloy
409Cb AWS A5.9 No
Mechanical Properties Carbon
0.010 Class EC409Cb
Required Manganese
.45 Silicon
0.55 Chromium
11.70 Niobium
0.60 Arcaloy 409Cb
is stabilized with columbium (niobium) for arc stability and to form carbides
as a means to improve corrosion resistance
and increase strength at high temperatures. Continued