COPYRIGHT 2000 THE ESAB GROUP, INC. LESSON
III 3.7.5
SUREWELD
SW612 (AWS
E6012) -
This is a multiple purpose rutile electrode that is
useful for poor fitup welding. It deposits convex weld beads that have great
resistance to cracking.
It withstands the high amperage of production welding without coating breakdown.
The weld deposit has excellent mechanical
properties for the classification. The SW612 electrode
is used to weld truck bodies, trailers, tanks, farm machinery and auto parts.
Typical mechanical properties are:
Yield Point - 62,300 psi
Tensile Strength - 69,400 psi
Elongation (2" Gauge) - 21%
Reduction of Area - 54%
The typical chemical composition of
the weld metal is: Carbon
0.05% Phosphorus
0.008% Manganese
0.31% Sulfur
0.016% Silicon
0.12% DEPOSITION
RATE DATA:
SW612*
Electrode Deposition
Diameter
Amperage
Efficiency,
% (Lbs/Hr.)
1/8" 130
81.8 2.9
5/32" 165
78.8 3.2
200 69.0
3.4 3/16"
220 77.0
4.0 250
74.5 4.2
7/32" 320
69.8 5.6
1/4" 320
70.0 5.6
360 67.7
6.6 380
66.0 7.1
*Note: Efficiencies do not include
stub loss